少妇人妻无码专区视频 I 久久精品国产精品 I 无码视频一区二区三区 I 国产精品久久久久久久久久免费 I 国产成人精品日本亚洲专区61 I 午夜天堂精品久久久久 I 欧美又大又色又爽aaaa片 I 激情综合亚洲色婷婷五月app I 国产精品天天狠天天看 I 中文 在线 日韩 亚洲 欧美 I 西西大胆午夜视频无码 I 国产精品无码免费播放 I 美女人妻激情乱人伦 I 神马午夜 I I 欧美一区 I 亚洲精品一区中文字幕乱码 I 亚洲 激情 小说 另类 欧美 I 蜜臀av在线播放 I 亚洲国产精品热久久 I a在线视频 I 天天色影网 I 欧美日韩精品 I 激情综合丁香五月 I 五十路熟妇亲子交尾

Test method for coating amount of PTP aluminum foil protective agent

Test method for coating amount of PTP aluminum foil protective agent

2022-12-12

Test method for coating amount of PTP aluminum foil protective agent

The protective agent layer of PTP aluminum foil is a dense cross-linked resin layer formed by high temperature curing. It is difficult to completely wipe the coating in a short time by the solvent wiping method commonly used now, and it is difficult to obtain accurate coating quantity value. Moreover, the repeatability of sample test results is also very poor. Therefore, a more effective test method for the coating quantity of PTP aluminum foil protective layer is found, It is of great practical value to guide the production of such products.

According to the material characteristics of PTP aluminum foil and the comparison of the advantages and disadvantages of various detection methods, we finally believe that the "burning method" is the most suitable for the rapid detection of the amount of protective agent coating:

In this method, the PTP aluminum foil sample is placed in a muffle furnace, maintained at a certain temperature for a certain time, and the PTP aluminum foil coated with the protective agent layer is baked at high temperature, so that the protective agent layer is completely oxidized and gasified. The coating amount of the protective agent layer can be calculated by detecting the quality of the aluminum foil before and after the high-temperature baking.

1、 Instruments and reagents:

10cm * 10cm standard cutting plate, blade, analytical balance (precision: 1/10000 g), muffle furnace, glass plate, stainless steel tweezers, ethyl acetate (analytical pure), absorbent cotton

2、 Test method:

1. Select the aluminum foil sample sheet for drug packaging with flat surface and no wrinkles, cut 5 test samples with a blade and a 10cm * 10cm standard cutting plate, and control the deviation of the width and length of the sample within ± 0.5mm

2. Weigh the cut sample (W1) on the balance.

3. Put the printing face of the aluminum foil on a glass plate, and use stainless steel tweezers to clamp the degreased cotton dipped in ethyl acetate to wipe the heat-sealing coating surface of the aluminum foil until no obvious marks can be identified when the surface is observed with naked eyes. (Note: The cotton ball dipped with ethyl acetate shall not have the liquid of ethyl acetate dripping. The circular wiping method from the center to the edge shall be used for wiping. The edge of the aluminum foil must be laid flat on the glass plate, and the linear wiping method shall be used for wiping. The other side of the aluminum foil shall not be affected during the whole process as much as possible). If the cotton ball has been wiped with the printing coating, replace it with a new cotton ball.

4. After wiping the heat-sealing coating, put the aluminum foil in a ventilated place and place it at room temperature for 2 minutes.

5. Then weigh the weight (W2) on the analytical balance

6. Place the above aluminum foil on the sample shelf in the muffle furnace preheated to 550-600 ℃. After waiting for a period of time, take out the coated aluminum foil and place it at room temperature. (The black ink may not completely volatilize the pigment, and its impact can be temporarily ignored for the products with general printed text patterns. If the printed patterns are large, the weight impact of the ink binder and the pigment should be considered)

7. Then weigh the weight (W3) on the analytical balance

Note: If the test sample has no adhesive layer, omit the operations in 2, 3 and 4.

8. Result calculation:

(W1-W2) × 100=weight of heat seal layer (g/m2)

(W2-W3) × 100=weight of printing layer/protective layer (g/m2) (when the sample has adhesive layer)

(W1-W3) × 100=weight of printing layer/protective layer (g/m2) (when the sample has no adhesive layer)

W3 × 100=weight of aluminum foil layer (g/m2)

Calculate and report the test results and average values of all individual samples to the nearest 0.01g/m2.


主站蜘蛛池模板: 免费永久看黄在线观看 | 欧美一进一出抽搐大尺度视频 | 久久亚洲中文字幕精品一区 | 国产精品综合色区在线观看 | 人妻系列av无码专区 | www.99tv| 狠狠躁夜夜躁av网站中文字幕 | 久久成人a毛片免费观看网站 | 久久久久日韩精品免费观看网 | 久久er99国产精品免费 | 少妇激情一区二区三区视频小说 | 久久国产劲爆∧v内射 | 国产成人精品一区二区三区视频 | 免费视频好湿好紧好大好爽 | 国产精品久久久久影院 | 尹人香蕉久久99天天拍久女久 | 伊人精品一本久久综合 | 亚洲精品国产av成拍色拍 | 一区二区三区乱码在线 | 欧洲 | 日韩一级免费免费视频 | 性色av免费在线观看 | 亚洲6080yy久久无码产自国产 | 亚洲国产精品一区二区成人片不卡 | 久久精品私人影院免费看 | 国产精品无码无片在线观看 | 中国凸偷窥xxxx自由视频 | 精品无码日韩国产不卡av | 亚洲成av人片在线观看高清 | 果冻传媒入口 | 亚洲精品无码成人网站 | 麻豆一区二区三区精品视频 | 成人高潮视频在线观看 | 性生交大全免费看 | 精品亚洲国产成人av在线 | 国产精品无码翘臀在线看 | 丰满大码的熟女在线视频 | 国产无遮挡裸体免费视频在线观看 | 无码精品人妻一区二区三区涩爱 | 狠狠色婷婷久久综合频道日韩 | 久久久久琪琪去精品色无码 | 国产av午夜精品一区二区三区 |